福建某铅锌浮选尾矿中铅、锌、银的品位分别为0.23%、2.11%、36.3 g/t,其中锌和银有较高回收价值。该尾矿中主要金属矿物为闪锌矿、黄铁矿和方铅矿,非金属矿物以方解石和石英为主。针对矿石特点,采用优先浮选开展工艺优化试验。结果表明:在磨矿细度为-0.074 mm占69.92%的条件下,以石灰为pH调整剂,硫酸锌为抑制剂,乙硫氮为捕收剂,2~#油为起泡剂,经1粗3精1扫浮铅,可获得铅品位4.56%、银品位320 g/t,铅回收率15.55%、银回收率6.63%的银铅精矿;针对选铅尾矿,以石灰为pH调整剂,硫酸铜为活化剂,丁基黄药为捕收剂,2~#油为起泡剂,经1粗3精2扫浮锌,可获得锌品位37.32%、银品位152 g/t,锌回收率73.25%、银回收率18.80%的锌精矿。试验指标较好,可为该尾矿的综合利用提供数据支撑。