Abstract:
在砂型铸造条件下.含 1.7~2.3%C、0.5~1.0%Si、0.4~1.0%Mn、0.3~0.7%Cr、0.3~0.7%Cu的白口铸铁磨球经1.0~1.5%1#稀土硅铁合金、0.1%A1处理,在800~900℃利用铸造余热水淬一定时间,并经280~350℃回火,硬度达HRC55以上.在有效高度为4.2m的磨球跌落试验机上.跌落破碎次数超过 5万次.DTM250/390球磨机工业应用试验结果表明.磨制无烟煤的吨煤磨球磨耗比稀土低碳白口铸铁磨球降低44.8%.
Keyword:
Reprint 's Address:
Email:
Source :
福州大学学报(自然科学版)
ISSN: 1000-2243
CN: 35-1337/N
Year: 1993
Issue: 02